Cronix 70 hutumika kwa vipengele vya kupokanzwa vya umeme vinavyostahimili kutu katika tanuu za viwandani zenye kupunguza angahewa. Cronix 70 ni sugu sana kwa oxidation katika hewa. Haipendekezwi kwa ajili ya matumizi katika vipengele vya kupokanzwa vilivyofunikwa na MgO, au programu zinazotumia nitrojeni au angahewa za kuziba.
Daraja | Ni80Cr20 | Ni70Cr30 | Ni60Cr23 | Ni60Cr15 | Ni35Cr20 | Karma | Evanohm | |
Utungaji mdogo% | Ni | Bal | Bal | 58.0-63.0 | 55.0-61.0 | 34.0-37.0 | Bal | Bal |
Cr | 20.0-23.0 | 28.0-31.0 | 21.0-25.0 | 15.0-18.0 | 18.0-21.0 | 19.0-21.5 | 19.0-21.5 | |
Fe | ≦1.0 | ≦1.0 | Bal | Bal | Bal | 2.0-3.0 | - | |
Al1.0-1.7 Ti 0.3-0.5 | Al2.7-3.2 Mn0.5-1.5 | Al2.7-3.2 Cu2.0-3.0 Mn0.5-1.5 | ||||||
Kiwango cha juu cha halijoto cha kufanya kazi (°C) | 1200 | 1250 | 1150 | 1150 | 1100 | 300 | 400 | |
Ustahimilivu(Ω/cmf,20℃) | 1.09 | 1.18 | 1.21 | 1.11 | 1.04 | 1.33 | 1.33 | |
Ustahimilivu (uΩ/m,60°F) | 655 | 704 | 727 | 668 | 626 | 800 | 800 | |
Uzito (g/cm³) | 8.4 | 8.1 | 8.4 | 8.2 | 7.9 | 8.1 | 8.1 | |
Uendeshaji wa Joto(KJ/m·h·℃) | 60.3 | 45.2 | 45.2 | 45.2 | 43.8 | 46.0 | 46.0 | |
Mgawo wa Upanuzi wa Mstari(×10¯6/℃)20-1000℃) | 18.0 | 17.0 | 17.0 | 17.0 | 19.0 | - | - | |
Kiwango Myeyuko(℃) | 1400 | 1380 | 1370 | 1390 | 1390 | 1400 | 1400 | |
Ugumu (Hv) | 180 | 185 | 185 | 180 | 180 | 180 | 180 | |
Nguvu ya Mkazo (N/mm2) | 750 | 875 | 800 | 750 | 750 | 780 | 780 | |
Kurefusha(%) | ≥20 | ≥20 | ≥20 | ≥20 | ≥20 | 10-20 | 10-20 | |
Muundo wa Micrographic | austenite | austenite | austenite | austenite | austenite | austenite | austenite | |
MagneticProperty | Sio | Sio | Sio | Kidogo | Sio | Sio | Sio | |
Maisha ya Haraka(h/℃) | ≥81/1200 | ≥50/1250 | ≥81/1200 | ≥81/1200 | ≥81/1200 | - | - |